甲基丙烯酸甲酯路面快速修补材料力学性能分析
叶飞1,啜二勇1*,刘路1,杨晓莹2
1.天津市交通科学研究院,天津 300300;2.中国长江三峡集团有限公司流域枢纽运行管理中心,湖北 宜昌 443133
摘要:为探究甲基丙烯酸甲酯(Methyl Methacrylate,MMA)胶凝材料配比,设计以丙烯酸异辛酯(2-Ethylhexyl Acrylate,2-EHA)及丙烯酸丁酯(n-butyl Acrylate,BA)两种软单体质量比、两种软单体与硬单体MMA质量比、引发剂过氧化苯甲酰(Benzoyl Peroxide,BPO)与所有单体质量比为变量的正交试验,分析胶凝材料浇铸体的固化时间、高低温性能和力学强度变化,并基于极差分析和灰色关联分析探究胶凝材料最佳配比;分析不同胶石比修补材料的抗压强度、抗弯拉强度和抗剪强度随龄期的变化趋势,并与水泥修补材料对比。研究结果表明:BPO引发剂质量与软硬单体总质量之比为2%,固化时间为20~30 min,可满足路面快速修补的现场施工操作要求;软单体与硬单体质量比为20%、2-EHA与BA质量比为3.0时,胶凝材料浇铸体的综合性能最优,玻璃化转变温度为123.3 ℃,温度为-12 ℃时,低温蠕变劲度模量为472 MPa,拉伸强度和弯曲强度分别为20.8、35.6 MPa,胶凝材料表面光滑无孔洞;以养护1.5 h为节点,前期MMA胶凝材料与集料质量比为11%的MMA快速修补材料的抗压强度增速较快,后期MMA胶凝材料与集料的质量比为10%的快速修补材料的抗压强度增速快,养护2.0 h快速修补材料的抗压强度为养护4.0 h快速修补材料的86.84%;MMA胶凝材料与集料的质量比为10%的MMA快速修补材料的养护1.0 h抗弯拉强度比养护0.5 h快速修补材料增大10.11%,养护2.0 h抗弯拉强度比养护1.5 h增大31.64%;不同MMA胶凝材料与集料质量比快速修补材料的初期抗剪强度达到养护4.0 h的77.4%;MMA快速修补材料的抗压强度和抗弯拉强度优于水泥修补料,但抗剪强度比水泥修补料小。
关键词:单体;胶凝材料配比;快速修补材料;固化时间;力学强度
Mechanical performance analysis of Methyl Methacrylate pavement rapid repair material
YE Fei1, CHUO Eryong1*, LIU Lu1, YANG Xiaoying2
1.Tianjin Transportation Research Institute, Tianjin 300300, China;
2.River Basin Complex Administration Center, China Three Gorges Corporation, Yichang 443133, China
Abstract: To investigate the proportion of MMA binder, an orthogonal experiment is designed with the mass ratios of 2-EHA and BA soft monomers, the total amount of soft monomers to the mass ratio of hard monomer MMA, and the dosage of BPO initiator as variables. The curing time, high and low temperature performance, and mechanical strength changes of the binder casting are analyzed, and the optimal proportion of binder is explored based on range analysis and grey correlation analysis; Subsequently, the evolution of compressive strength, flexural-tensile strength, and shear strength in repair materials with different MMA binder dosages during curing is examined and compared with cementitious repair materials. The results show that BPO initiator mBPO/(m2-EHA+mBA+mMMA)= 2%, and the curing time is maintained at 20-30 min, can meet the on-site construction operation requirements for rapid pavement repair; When (m2-EHA+mBA)/mMMA is 20% and w1=3, the comprehensive properties of the binder casting body is optimal, with a glass transition temperature reaching 123.3 ℃, a low-temperature creep stiffness modulus of 472 MPa at -12 ℃, and tensile strength and flexural strength reaching 20.8 MPa and 35.6 MPa, respectively. The surface of the bonding material is smooth without any holes appearing. Taking 1.5 h as the node, the MMA repair material with an 11% binder-to-aggregate mass ratio exhibits a faster compressive strength development rate in the early stage, while the 10% binder-to-aggregate mass ratio MMA repair material shows accelerated strength gain in the later stage; At 2.0 h, 10% binder-to-aggregate mass ratio repair material compressive strength reaches 86.84% of the 4.0 h strength; The flexural tensile strength of MMA repair material with 10% binder-to-aggregate mass ratio after 1.0 h of curing increase by 10.11% compared to 0.5 h of curing, and the flexural tensile strength after 2.0 h of curing increase by 31.64% compared to 1.5 h of curing; The initial shear strength of repair materials with different mass ratios of binder-to-aggregate reaches 77.4% of the 4.0 h shear strength; The compressive strength and flexural tensile strength of MMA rapid repair material are better than those of cement repair material, while the shear strength is lower than cement repair material.
Keywords: monomer; binder mix proportion; rapid repair material; curing time; mechanical strength